Spool OD roughness had to be Ra 0.2–0.4 µm and every reading was inside that band, yet bench leakage stayed high, suggesting many peaks and little bearing area.
Solution: CX-3/100 measuring Rmr, Rpk and Rvk alongside Ra/Rz to ISO 13565 for plateau assessment, plus profile roundness and straightness.
Result: Ra 0.31 µm passed but Rmr(2cr) was only 42% against a 60% requirement, a classic unremoved-peak condition; after changing honing stone grit and stroke speed Rmr reached 68%, leakage dropped 60% and bench first-pass rate rose from 72% to 96%.