HXZMP-3000 Smart fully automatic metallographic grinder-polisher
Complete metallographic specimen preparation
- Control双盘磨抛,压力/转速/时间可编程
- Cooling循环冷却,试样温度可控

Complete metallographic specimen preparation

Complete metallographic specimen preparation

Complete metallographic specimen preparation

Complete metallographic specimen preparation

Complete metallographic specimen preparation

Complete metallographic specimen preparation

Complete metallographic specimen preparation

Complete metallographic specimen preparation

Complete metallographic specimen preparation

Complete metallographic specimen preparation

Complete metallographic specimen preparation

Complete metallographic specimen preparation

Complete metallographic specimen preparation

Complete metallographic specimen preparation

Complete metallographic specimen preparation

Complete metallographic specimen preparation
Metallographic Preparation
The goal of metallographic preparation is a flat, scratch-free mirror with intact edges and unchanged microstructure. The sequence is sectioning → mounting → grinding → polishing → etching, and every step affects the result.
Sectioning: diamond or alumina wheels with constant feed and abundant coolant to avoid heat-affected zones and deformation. Soft materials use resin-bonded wheels, hard materials metal-bonded diamond.
Mounting: hot mounting (phenolic, 130–180 °C, 20–30 MPa) is fast; cold mounting (epoxy/acrylic) suits temperature-sensitive materials and edge retention; copper-filled mounts allow electrolytic polishing.
Grinding and polishing: remove scratches step by step, each step fully erasing the previous one; diamond suspension 3 µm then 1 µm, final oxide polish. Soft materials need low pressure and short times to avoid relief.
Metallographic Preparation
Metallographic Preparation
1. Grinding allowance: each grade must remove 3–4× the previous scratch depth — 20–30 µm per grade (320→1200) for carbon steel; rotate the sample 90° at each change.
2. Burn-free cutting: keep feed low enough that chips do not blue (~300 °C); burned layers shift surface hardness by 2–5 HRC and show as tempered zones.
3. Hot mounting: phenolic at 150–165 °C, 250–300 bar, 5–8 min; use cold epoxy (24 °C/24 h or accelerated 60 °C/1 h) for quenched or aluminium parts.
4. Polishing time: removal ∝ P·n; typical 2–3 min at 3 µm diamond and 1–2 min at 1 µm — excess pressure causes smearing and pitting.
5. Etching quota: 4% nital 3–8 s for carbon steel; fix time, temperature and concentration per batch for comparability.
Metallographic Preparation
| Standard | Title | Use |
|---|---|---|
| ASTM E3-11 | Guide for metallographic specimen preparation | Preparation workflow |
| GB/T 13298-2015 | Examination of microstructure | General inspection |
| GB/T 15749-2008 | Quantitative metallography | Quantitative analysis |
| GB/T 10561-2005 | Non-metallic inclusion content in steel | Inclusions |
| ISO 4967 | Determination of non-metallic inclusions | Export projects |
Metallographic Preparation
1. Four linked steps: sectioning without deformation, mounting without voids and with edge protection, polishing without scratches or rounding, then etching and observation. A wrong choice at any step cannot be rescued by a better microscope.
2. Cutter by section size and heat sensitivity: abrasive cutters (HXQ-50/HXQ-100) for routine parts; low-speed precision sectioning with diamond or CBN wheels below 300 rpm for coatings, sheet and non-ferrous.
3. Mounting by batch and edge requirements: hot mounting (HXZDQ) is fast and cheap for routine parts; cold vacuum impregnation suits porous, coated and electronic samples.
4. Polishing by throughput: manual (HXZMP-1000) below 20 samples a day, semi-automatic (HXZMP-2000) for 20–80, automatic heads (HXZMP-3000) above 80 or where consistency matters.
5. Consumables matter more than the machine: grit sequence 180→400→800→1200→2000, diamond suspension 9→3→1 µm and the right cloth type must match, or you either cannot polish out or polish past the feature.
6. Room and safety: extraction and water for cutting and polishing, separate preparation and microscopy rooms, guards and e-stops on cutters.
| Equipment | Model | Capability | Use |
|---|---|---|---|
| Precision cutter | HXQ-50 / HXQ-100 | Low speed, no deformation | Coatings, sheet, non-ferrous |
| Abrasive cutter | HXGXS | Fast large-section cutting | Routine steel parts |
| Hot mounting press | HXZDQ-100 / 110 / 120 / 160 | Φ25–Φ50 mounts | Batch routine samples |
| Vacuum mounting | HXZDQ-100Z | Vacuum impregnation | Porous, coated, electronics |
| Manual polisher | HXZMP-1000 | Single platen | Low volume, teaching |
| Semi-automatic | HXZMP-2000 / 2000Z | Twin platen, timed | Medium batches |
| Automatic | HXZMP-3000 | Multi-station, programmable force | High throughput, consistency |
| Electrolytic polish/etch | HXSQ-100G / 100F | Deformation-free surface | Stainless, nickel alloys |
Why samples get scrapped: cutting heat alters the structure, mounting gaps cause edge smearing, over-polishing removes inclusions, over-etching blurs grain boundaries.
Metallographic Preparation
Sampling. Choose a representative section (gear root, weld cross-section), cut perpendicular to the viewing plane, and record position and orientation.
Cutting. 0.5–2 mm/min feed, 2000–3000 rpm, abundant coolant; re-section if burn marks appear.
Mounting. Hot mount at 150 °C, 25 MPa for 8 min; cold epoxy cure 4 h (or 60 °C acceleration). Add a protective plate for coating cross-sections to prevent rounding.
Grinding and polishing. 320→600→800→1200, rinse and rotate 90° between steps; diamond 3 µm (3 min), 1 µm (2 min), oxide (1 min), decreasing force.
Check. Inspect unetched at 100× for scratches and edge rounding, then etch. Verify preparation quality daily with a reference sample.
Metallographic Preparation

Precision sectioning plus vacuum mounting delivers results in 35 minutes with …

Low-speed sectioning with vacuum mounting and electrolytic polishing cut coati…

HXZDQ-160 mounting with HXZMP-3000 automatic polishing completes six samples i…

An HXZDQ-160 + HXQ-100 + HXZMP-2000 line raised PQR section acceptance from 85…

Q-2 saw, XQ-2B press and MP-2 dual platen raised output from 40 to 85 samples …

HXZDQ-100Z low-speed precision cutting prevents burn on SLM TC4 coupons; with …