Surface engineering2024

Cross-section preparation of thermal-spray coatings with edge protection

Low-speed sectioning with vacuum mounting and electrolytic polishing cut coating thickness deviation from 12% to 2% and raised porosity agreement to 95%.

Firma
Aviation coatings company, Shaanxi
Adresse
Xian, Shaanxi
Cross-section preparation of thermal-spray coatings with edge protection
12% → 2%Thickness deviation
70% → 95%Porosity agreement
无倒角Edge

HVOF WC-Co coatings are 200–400 µm thick and the edges round easily during thickness and porosity measurement. Conventional hot mounting and manual polishing produced rounded edges, thickness reading 10% low and porosity polished away.

Solution: HXQ-50 low-speed sectioning at 180 rpm with a diamond wheel, vacuum mounting of sample plus support plate in epoxy at -0.09 MPa (HXZDQ-100Z), stepped grinding and polishing, then 15 seconds of electrolytic polishing to remove the deformed layer.

Result: thickness deviation down from 12% to 2% with straight edges, and three-operator agreement on porosity from 70% to 95%; the method is now used in the company coating qualification.

⇄0VergleichTechnischer Vergleich