The centre handles 40–60 bolts a day for decarburisation, carburisation and laps. Single-platen manual polishing took 25 minutes per piece, two inspectors managed 30 a day, and uneven hand pressure skewed decarburisation readings.
Solution: HXQ-50 precision sectioning to avoid overheating, HXZDQ-160 mounting six at a time, HXZMP-3000 automatic polishing with four grinding and two diamond steps under programmed force and time, then 4% nital etch.
Result: six samples in 40 minutes, about 6.7 minutes each, raising daily throughput from 30 to 110; decarburisation repeatability within 0.01 mm; one inspector now handles preparation while the other moves to data analysis.