Foundry and metallurgy2023

Metallographic nodularity rating of ductile iron

MMAS-4 rates QT450-10 nodularity per GB/T 9441 at the furnace in 15 minutes, replacing 2-day outsourcing.

회사명
An auto parts foundry, E. China
주소
Anhui
카테고리
Microscopes
Metallographic nodularity rating of ductile iron
2 d → 15 minJudgment cycle
1.8% → 0.3%Scrap rate

Nodularity was judged by outsourced metallography with a 2-day delay, so failed heats had already been poured into castings, costing over one million RMB per year.

Solution: the MMAS-4 inverted metallurgical microscope with a furnace-side rapid polishing stand rates graphite morphology per GB/T 9441 at 100X on unetched samples, with 500X verification of pearlite; 2 samples per heat, 5 fields each.

Result: judgment time fell from 2 days to 15 minutes, with 98% agreement against third-party labs for grade 3 and above. Scrap from poor nodularization fell from 1.8% to 0.3% in the same year.

⇄0비교사양 비교