Wind-tower high-strength bolts must reach KV2 of at least 27 J at -40 ℃. The manual pendulum with a dry-ice bath gave uneven temperatures, specimens warmed quickly after removal, and three-piece sets often spread more than 10 J, which the owner rejected.
Solution: a JBS-300Z/500Z automatic pendulum impact tester with 300/500 J dual ranges and automatic specimen feeding, plus a CDW-60 cascade-compressor bath holding -40 ℃ within ±0.5 ℃. The specimen travels from bath to strike within 5 seconds, meeting GB/T 229.
Result: 10.9-grade bolts measured 38, 41 and 39 J KV2 at -40 ℃, a 3 J spread; the tester passed verification to GB/T 3808.
Benefit: the low-temperature impact data were accepted by the owner at first submission, and bolt-lot release time was cut in half.