Gold-plated terminals were judged by XRF to have Ni underlayer below 1.5 μm (contract ≥2 μm); the supplier questioned XRF accuracy on curved surfaces and the lot faced return.
Solution: the BIAS-400 system applied ASTM B487 cross-section arbitration: cold-mounted terminals polished to mid-section, Au and Ni thicknesses measured at 1000X, 5 points averaged per part, compared point-by-point with XRF.
Result: the cross-section method showed 2.3-2.6 μm Ni, meeting the contract; XRF read 30% low at terminal radii due to insufficient curvature correction. Both parties adopted the cross-section method for incoming inspection.