Điện tử đầu nối2024

Đo lớp nền Ni đầu nối mạ vàng

BIAS-400 đo lớp Ni 2,3 μm theo ASTM B487, sai lệch XRF ≤8%.

Công ty
Nhà máy đầu nối, Đông Trung Quốc
Địa chỉ
Giang Tô
Danh mục
Kính hiển vi
Đo lớp nền Ni đầu nối mạ vàng
2.3 μmĐộ dày lớp Ni

Gold-plated terminals were judged by XRF to have Ni underlayer below 1.5 μm (contract ≥2 μm); the supplier questioned XRF accuracy on curved surfaces and the lot faced return.

Solution: the BIAS-400 system applied ASTM B487 cross-section arbitration: cold-mounted terminals polished to mid-section, Au and Ni thicknesses measured at 1000X, 5 points averaged per part, compared point-by-point with XRF.

Result: the cross-section method showed 2.3-2.6 μm Ni, meeting the contract; XRF read 30% low at terminal radii due to insufficient curvature correction. Both parties adopted the cross-section method for incoming inspection.