304 stainless welded pipe needs metallographic checks of weld structure and ferrite content before shipping. The grinder and polisher sat in separate rooms, samples shuttled between them, and scratches at the fusion line were misread by a customer as lack-of-fusion defects.
Solution: an HXZMP-1000 combined grinder-polisher runs 240, 600 and 1200 grit papers then 3 um and 1 um diamond; electrolytic etching in 10% oxalic acid at 6 V for 15 s reveals weld dendrites, HAZ and base metal in one field.
Results: fusion-line boundaries are clean and artefact-free; ferrite measures 6.2% by point counting, inside the 3-10% process window. Prep throughput doubled to 40 weld samples a day, and annual customer quality disputes fell from six to one.