Hydraulic castings2025

Quantitative porosity analysis of HPDC valve bodies

MMAS-8 measured 1.8% porosity per ASTM E562 point counting; after fixing the intensification profile, pressure-test yield returned to 99.2%.

Firma
A hydraulic valve manufacturer, E. China
Adresse
Zhejiang
Kategorie
Microscopes
Quantitative porosity analysis of HPDC valve bodies
1.8% → 0.7%Porosity
99.2%Pressure-test yield

Three percent of 35 MPa high-pressure valve bodies leaked in pressure testing while X-ray spot checks showed nothing obvious; quantitative porosity data was needed.

Solution: the MMAS-8 metallographic system sampled sections along the main oil gallery and applied ASTM E562 point counting over 50 grid fields at 100X, grading pores by maximum diameter.

Result: the leaking lot showed 1.8% porosity with 380 μm maximum pores concentrated at the far end of the intensification zone. After adjusting the intensification profile and pouring temperature, porosity fell to 0.7% and first-pass yield recovered from 97% to 99.2%.

⇄0VergleichTechnischer Vergleich