Гидравлические отливки2025

Количественный анализ пористости корпусов клапанов

MMAS-8: пористость 1,8% по ASTM E562, выход годных 99,2%.

Компания
Производитель гидроклапанов, Вост. Китай
Адрес
Чжэцзян
Категория
Микроскопы
Количественный анализ пористости корпусов клапанов
1.8% → 0.7%Пористость
99.2%Выход по опрессовке

Three percent of 35 MPa high-pressure valve bodies leaked in pressure testing while X-ray spot checks showed nothing obvious; quantitative porosity data was needed.

Solution: the MMAS-8 metallographic system sampled sections along the main oil gallery and applied ASTM E562 point counting over 50 grid fields at 100X, grading pores by maximum diameter.

Result: the leaking lot showed 1.8% porosity with 380 μm maximum pores concentrated at the far end of the intensification zone. After adjusting the intensification profile and pouring temperature, porosity fell to 0.7% and first-pass yield recovered from 97% to 99.2%.

⇄0СравнениеСравнение характеристик