Đúc thủy lực2025

Phân tích độ rỗng thân van đúc

MMAS-8 đo độ rỗng 1,8% theo ASTM E562, tỷ lệ đạt 99,2%.

Công ty
Nhà máy van thủy lực, Đông Trung Quốc
Địa chỉ
Chiết Giang
Danh mục
Kính hiển vi
Phân tích độ rỗng thân van đúc
1.8% → 0.7%Độ rỗng
99.2%Tỷ lệ đạt thử áp

Three percent of 35 MPa high-pressure valve bodies leaked in pressure testing while X-ray spot checks showed nothing obvious; quantitative porosity data was needed.

Solution: the MMAS-8 metallographic system sampled sections along the main oil gallery and applied ASTM E562 point counting over 50 grid fields at 100X, grading pores by maximum diameter.

Result: the leaking lot showed 1.8% porosity with 380 μm maximum pores concentrated at the far end of the intensification zone. After adjusting the intensification profile and pouring temperature, porosity fell to 0.7% and first-pass yield recovered from 97% to 99.2%.

⇄0So sánhSo sánh thông số