Mould industry2024

HXZDQ-120 Burn-Free Cutting of H13 Nitrided Layers

HXZDQ-120 wet metallographic cutting with low feed keeps the burn layer within 3 um on H13 nitrided samples; the 8 um white layer and 0.15 mm diffusion zone measure undistorted, halving nitriding qualification time.

Firma
A die-casting mould heat treater, S. China
Adresse
Foshan, Guangdong
HXZDQ-120 Burn-Free Cutting of H13 Nitrided Layers
≤3 μmCut burn layer
8 μmWhite layer depth

After gas nitriding of H13 die-casting dies, white layer and diffusion zone depths must be measured. Aggressive abrasive cutting left a 20 um burn layer that etched away the white layer, so it was misread as having no compound layer and qualification took three rounds.

Solution: an HXZDQ-120 metallographic cutter with water cooling and a low 0.05 mm/s feed keeps the burn layer within 3 um. Edge-protecting hot mounts are polished to 1 um and etched in 4% nital, then white layer and diffusion depths are read at 500X.

Results: the 8 um white layer and 0.15 mm diffusion zone measure cleanly, agreeing with HV0.3 microhardness gradient mapping. Nitriding qualification fell from three rounds to one, early soldering on dies dropped 40%, and trial cost per die fell by 18000 yuan.

⇄0VergleichTechnischer Vergleich