Контроль поверхностной термообработки2024

Арбитражное измерение глубины азотирования 38CrMoAl

HMM-240S: глубина азотирования 0,42 мм по GB/T 11354 для арбитража.

Компания
Центр термообработки, Вост. Китай
Адрес
Цзянсу
Категория
Микроскопы
Арбитражное измерение глубины азотирования 38CrMoAl
0.42 mmИзмеренная глубина

Nitrided 38CrMoAl spindles were rejected by the customer on hardness-method case depth (spec ≥0.40 mm); the method dispute threatened a full-lot return.

Solution: the HMM-240S metallurgical microscope applied the arbitration method of GB/T 11354: after etching with 4% nital, the perpendicular depth from surface to core boundary was measured at 500X, averaging 3 fields per part.

Result: metallographic case depth was 0.42-0.45 mm, meeting the contract; the dispute came from the customer’s excessive hardness load piercing the compound layer. The arbitration report was accepted by both parties.

⇄0СравнениеСравнение характеристик