Kiểm tra nhiệt luyện bề mặt2024

Đo trọng tài chiều sâu lớp thấm nitơ 38CrMoAl

HMM-240S đo lớp thấm nitơ 0,42 mm theo GB/T 11354 làm trọng tài.

Công ty
Trung tâm nhiệt luyện, Đông Trung Quốc
Địa chỉ
Giang Tô
Danh mục
Kính hiển vi
Đo trọng tài chiều sâu lớp thấm nitơ 38CrMoAl
0.42 mmChiều sâu đo được

Nitrided 38CrMoAl spindles were rejected by the customer on hardness-method case depth (spec ≥0.40 mm); the method dispute threatened a full-lot return.

Solution: the HMM-240S metallurgical microscope applied the arbitration method of GB/T 11354: after etching with 4% nital, the perpendicular depth from surface to core boundary was measured at 500X, averaging 3 fields per part.

Result: metallographic case depth was 0.42-0.45 mm, meeting the contract; the dispute came from the customer’s excessive hardness load piercing the compound layer. The arbitration report was accepted by both parties.

⇄0So sánhSo sánh thông số