HMM-240S measured a 0.42 mm nitrided case per GB/T 11354 as arbitration evidence in a hardness-method dispute, avoiding lot rejection.

Company
A heat treatment job shop, E. China
Address
Jiangsu
Category
Microscopes
Arbitration measurement of nitrided case depth on 38CrMoAl
0.42 mmMeasured case depth

Nitrided 38CrMoAl spindles were rejected by the customer on hardness-method case depth (spec ≥0.40 mm); the method dispute threatened a full-lot return.

Solution: the HMM-240S metallurgical microscope applied the arbitration method of GB/T 11354: after etching with 4% nital, the perpendicular depth from surface to core boundary was measured at 500X, averaging 3 fields per part.

Result: metallographic case depth was 0.42-0.45 mm, meeting the contract; the dispute came from the customer’s excessive hardness load piercing the compound layer. The arbitration report was accepted by both parties.