Automotive gears2022

Macro flow-line inspection of transmission gear forgings

MMAS-6 inspected forging flow lines per GB/T 226 macro etching; after preform-die optimization for cut flow lines at tooth roots, fatigue life rose 28%.

회사명
A gear forging plant, S. China
주소
Guangdong
카테고리
Microscopes
Macro flow-line inspection of transmission gear forgings
+28%Fatigue life gain

Gear forgings for a transmission plant fell short of the 220k-cycle tooth-root bending fatigue target; fracture analysis pointed to abnormal flow-line distribution.

Solution: the MMAS-6 microscope applied GB/T 226 hot macro-etching; at 50X, stitched images of the tooth-root fillet judged flow direction and cut locations, driving three iterations of the preform-die fillet.

Result: in the original design 30% of roots had flow lines cut by flash. Enlarging the preform fillet from R3 to R6 made flow lines continuously envelop the root, raising bench fatigue life to 280k cycles.

⇄0비교사양 비교