Автомобильные шестерни2022

Макроконтроль волокон поковок шестерён

MMAS-6: волокна поковок по GB/T 226, ресурс вырос на 28%.

Компания
Кузнечный завод шестерён, Юж. Китай
Адрес
Гуандун
Категория
Микроскопы
Макроконтроль волокон поковок шестерён
+28%Рост ресурса

Gear forgings for a transmission plant fell short of the 220k-cycle tooth-root bending fatigue target; fracture analysis pointed to abnormal flow-line distribution.

Solution: the MMAS-6 microscope applied GB/T 226 hot macro-etching; at 50X, stitched images of the tooth-root fillet judged flow direction and cut locations, driving three iterations of the preform-die fillet.

Result: in the original design 30% of roots had flow lines cut by flash. Enlarging the preform fillet from R3 to R6 made flow lines continuously envelop the root, raising bench fatigue life to 280k cycles.

⇄0СравнениеСравнение характеристик