Bánh răng ô tô2022

Kiểm tra vân rèn bánh răng hộp số

MMAS-6 kiểm vân rèn theo GB/T 226, tuổi thọ tăng 28%.

Công ty
Nhà máy rèn bánh răng, Nam Trung Quốc
Địa chỉ
Quảng Đông
Danh mục
Kính hiển vi
Kiểm tra vân rèn bánh răng hộp số
+28%Tăng tuổi thọ mỏi

Gear forgings for a transmission plant fell short of the 220k-cycle tooth-root bending fatigue target; fracture analysis pointed to abnormal flow-line distribution.

Solution: the MMAS-6 microscope applied GB/T 226 hot macro-etching; at 50X, stitched images of the tooth-root fillet judged flow direction and cut locations, driving three iterations of the preform-die fillet.

Result: in the original design 30% of roots had flow lines cut by flash. Enlarging the preform fillet from R3 to R6 made flow lines continuously envelop the root, raising bench fatigue life to 280k cycles.