Automotive2023

MARSURF-XCR20 for Plateau Honing Rk Control of Liners

MARSURF-XCR20 evaluates Rk, Rpk and Rvk of plateau honing per ISO 13565-2; tightening Rvk to 0.8±0.2 um cut oil consumption by 30%.

회사명
An engine cylinder liner maker, C. China
주소
Xiangyang, Hubei
MARSURF-XCR20 for Plateau Honing Rk Control of Liners
0.8±0.2 μmRvk window
30%Oil consumption cut

Liner honing was controlled by Ra 0.2-0.4 um alone. Bores with identical Ra differed greatly in oil retention; the engine customer reported high oil consumption on some batches and a 0.3% scuffing rate during run-in.

Solution: a MARSURF-XCR20 roughness and contour instrument with a 2 um diamond stylus, evaluating the material-ratio curve parameters Rk, Rpk, Rvk, Mr1 and Mr2 per ISO 13565-2. Three axial traces per bore with a 0.8 mm x 5 sampling scheme replaced the single Ra check.

Results: with the process window reset to Rvk 0.8±0.2 um and Rpk ≤0.3 um, batch scatter of groove depth shrank by 60%, engine oil consumption dropped 30%, and run-in scuffing fell from 0.3% to 0.05%.