MARSURF-XCR20 kiểm soát Rk mài nghiền xy lanh

MARSURF-XCR20 đánh giá Rk, Rpk, Rvk theo ISO 13565-2; siết Rvk 0,8±0,2 um giảm 30% tiêu hao dầu.

Công ty
Nhà máy xy lanh, Trung Trung Quốc
Địa chỉ
Tương Dương, Hồ Bắc
MARSURF-XCR20 kiểm soát Rk mài nghiền xy lanh
0.8±0.2 μmCửa sổ Rvk
30%Giảm tiêu hao dầu

Liner honing was controlled by Ra 0.2-0.4 um alone. Bores with identical Ra differed greatly in oil retention; the engine customer reported high oil consumption on some batches and a 0.3% scuffing rate during run-in.

Solution: a MARSURF-XCR20 roughness and contour instrument with a 2 um diamond stylus, evaluating the material-ratio curve parameters Rk, Rpk, Rvk, Mr1 and Mr2 per ISO 13565-2. Three axial traces per bore with a 0.8 mm x 5 sampling scheme replaced the single Ra check.

Results: with the process window reset to Rvk 0.8±0.2 um and Rpk ≤0.3 um, batch scatter of groove depth shrank by 60%, engine oil consumption dropped 30%, and run-in scuffing fell from 0.3% to 0.05%.