Two AlTiN coating formulations had equal room-temperature hardness, yet tool life in dry cutting of superalloys differed by a factor of two, with no direct evidence at cutting temperature.
Solution: IMAS-HT700CM applied 50 gf micro-indents on coating cross-sections at 800℃ (indent depth below 1/10 of film thickness), 10 points per formulation, hardness converted per ISO 14577 with substrate correction.
Result: the high-Al formulation retained 61% of its hardness at 800℃ versus 42% for the standard one, matching the 2.1:1 tool-life ratio. The data justified designating the high-Al grade for dry cutting of superalloys.