Производство режущего инструмента2025

Твердость покрытия AlTiN при 800℃

IMAS-HT700CM: микроиндентирование AlTiN при 800℃, удержание твердости выросло с 42% до 61%.

Компания
Производитель инструмента с ЧПУ, Вост. Китай
Адрес
Цзянсу
Твердость покрытия AlTiN при 800℃
42% → 61%Удержание твердости при 800℃

Two AlTiN coating formulations had equal room-temperature hardness, yet tool life in dry cutting of superalloys differed by a factor of two, with no direct evidence at cutting temperature.

Solution: IMAS-HT700CM applied 50 gf micro-indents on coating cross-sections at 800℃ (indent depth below 1/10 of film thickness), 10 points per formulation, hardness converted per ISO 14577 with substrate correction.

Result: the high-Al formulation retained 61% of its hardness at 800℃ versus 42% for the standard one, matching the 2.1:1 tool-life ratio. The data justified designating the high-Al grade for dry cutting of superalloys.

⇄0СравнениеСравнение характеристик