Nuclear power2022

500℃ hardness monitoring of irradiated RPV steel

HMAS-HT600 measured irradiated SA508-3 at 500℃ inside a hot cell, tracking thermal recovery of irradiation hardening for life assessment.

Firma
A nuclear safety research institute, E. China
Adresse
Shanghai
500℃ hardness monitoring of irradiated RPV steel
31%Hardening recovery

The institute needed to quantify irradiation hardening of RPV surveillance specimens near the upper-shelf service temperature inside a hot cell, beyond the capability of ordinary hardness testers.

Solution: HMAS-HT600 with remote-handling fixtures made ten 1 kgf indents at 500℃ on pre- and post-irradiation SA508-3 samples, 15 s dwell, images acquired through a lead-glass window with a long-working-distance objective, calculated per GB/T 4340.1.

Result: the 500℃ hardness increment after irradiation was 38 HV versus 55 HV at room temperature, i.e. 31% recovery. The recovery law was included in the 60-year life-extension justification.

⇄0VergleichTechnischer Vergleich