Điện hạt nhân2022

Độ cứng thép vỏ lò phản ứng ở 500℃

HMAS-HT600 đo thép SA508-3 chiếu xạ ở 500℃ trong buồng nóng.

Công ty
Viện an toàn hạt nhân, Đông Trung Quốc
Địa chỉ
Thượng Hải
Độ cứng thép vỏ lò phản ứng ở 500℃
31%Tỷ lệ hồi phục hóa cứng

The institute needed to quantify irradiation hardening of RPV surveillance specimens near the upper-shelf service temperature inside a hot cell, beyond the capability of ordinary hardness testers.

Solution: HMAS-HT600 with remote-handling fixtures made ten 1 kgf indents at 500℃ on pre- and post-irradiation SA508-3 samples, 15 s dwell, images acquired through a lead-glass window with a long-working-distance objective, calculated per GB/T 4340.1.

Result: the 500℃ hardness increment after irradiation was 38 HV versus 55 HV at room temperature, i.e. 31% recovery. The recovery law was included in the 60-year life-extension justification.

⇄0So sánhSo sánh thông số