Some GH4169 bolt lots lost preload early after assembly although room-temperature hardness passed; the root cause could not be located.
Solution: HMAS-HT700CM performs 5 kgf Vickers indents on 5 bolts per heat lot at 650℃ (the service temperature), 15 min soaking, 12 s dwell, HV5 conversion per GB/T 4340.1, with an SPC database per lot.
Result: two lots with low solution temperature showed 650℃ hardness 11% below the floor, matching the failed bolts exactly. Lot scatter tightened from ±8% to ±3% and zero-kilometer complaints dropped to zero.