Fastener manufacturing2023

650℃ hardness consistency control of superalloy bolts

HMAS-HT700CM samples 5 GH4169 bolts per heat lot at 650℃ per GB/T 4340.1; hardness scatter tightened from ±8% to ±3%.

会社名
An aerospace fastener plant, N. China
所在地
Beijing
650℃ hardness consistency control of superalloy bolts
±8% → ±3%Hardness scatter

Some GH4169 bolt lots lost preload early after assembly although room-temperature hardness passed; the root cause could not be located.

Solution: HMAS-HT700CM performs 5 kgf Vickers indents on 5 bolts per heat lot at 650℃ (the service temperature), 15 min soaking, 12 s dwell, HV5 conversion per GB/T 4340.1, with an SPC database per lot.

Result: two lots with low solution temperature showed 650℃ hardness 11% below the floor, matching the failed bolts exactly. Lot scatter tightened from ±8% to ±3% and zero-kilometer complaints dropped to zero.