Разъёмы2025

Партийный контроль микротвёрдости пружин из БрБ

HVS-1000Z: пружины БрБ 0,15 мм при HV0.2, 380 HV, разброс ≤15 HV.

Компания
Завод разъёмов, Вост. Китай
Адрес
Юэцин, Чжэцзян
Категория
Твердомеры
Партийный контроль микротвёрдости пружин из БрБ
380 HV0.2Твёрдость после старения
1 周 → 当天Срок контроля

The 0.15 mm beryllium-copper contact springs in high-speed connectors get their contact force from ageing hardness. Outsourced testing took a week, and uneven clamping of the thin strip made readings jump around.

Solution: an HVS-1000Z digital micro-Vickers hardness tester at HV0.2 (1.961 N) with 10 s dwell, using a vacuum thin-foil holder to keep the strip level. Indentation spacing of at least 2.5 diagonals per GB/T 4340.1 is placed automatically.

Result: 380 HV0.2 after ageing with a 10-point lot spread within 15 HV; hardness correlated with measured spring force at r = 0.93, so rapid hardness checks now replace part of the full force testing.

Benefit: turnaround fell from a week to same-day, and lot-consistency complaints on springs dropped 70%.

⇄0СравнениеСравнение характеристик