Steel and metallurgy2023

600℃ red-hardness grading of HSS work rolls

HMAS-HT800 grades HSS work rolls by 600℃ red hardness per GB/T 4340.1 instead of room-temperature hardness alone.

회사명
A roll manufacturer, N. China
주소
Hebei
600℃ red-hardness grading of HSS work rolls
+22%Tonnage gain

HSS work rolls with identical room-temperature hardness behaved very differently in hot strip mills; complaints centered on spalling and early wear.

Solution: HMAS-HT800 makes five 10 kgf indents at 600℃ (near roll-surface working temperature) on the end test ring of every roll, 15 s dwell, HV10 per GB/T 4340.1; a 600℃ retention ratio ≥55% is set as the Grade-A shipping threshold.

Result: Grade-A rolls achieved 22% higher average tonnage and spalling complaints fell 80%. Red-hardness data is now printed on the quality certificate as a settlement index with the mill.

⇄0비교사양 비교