Aircraft manufacturing2024

Microstructure rating of TC4 EB welds

MMAS-12 rated α-lath structure of TC4 EB welds per HB 5276; optimized focus current raised joint efficiency to 0.96.

Company
An aircraft structures plant, NW China
Address
Shaanxi
Category
Microscopes
Microstructure rating of TC4 EB welds
0.96Joint efficiency

Joint efficiency of TC4 load-frame EB welds fluctuated between 0.88 and 0.95, failing to stably meet the 0.92 design floor; the link between weld microstructure and parameters was missing.

Solution: the MMAS-12 research microscope (incident/transmitted light) rated weld sections per HB 5276, measuring α-lath width and basketweave fraction at 500X across six focus-current settings.

Result: excessive focus current coarsened α laths (2.8 μm average) and caused the strength scatter. After optimization, lath width was 1.6 μm, joint efficiency stabilized at 0.96, and production yield reached 100%.