Chế tạo hàng không2024

Đánh giá tổ chức mối hàn TC4

MMAS-12 đánh giá mối hàn TC4 theo HB 5276, hệ số bền 0,96.

Công ty
Nhà máy kết cấu hàng không, Tây Bắc Trung Quốc
Địa chỉ
Thiểm Tây
Danh mục
Kính hiển vi
Đánh giá tổ chức mối hàn TC4
0.96Hệ số bền mối hàn

Joint efficiency of TC4 load-frame EB welds fluctuated between 0.88 and 0.95, failing to stably meet the 0.92 design floor; the link between weld microstructure and parameters was missing.

Solution: the MMAS-12 research microscope (incident/transmitted light) rated weld sections per HB 5276, measuring α-lath width and basketweave fraction at 500X across six focus-current settings.

Result: excessive focus current coarsened α laths (2.8 μm average) and caused the strength scatter. After optimization, lath width was 1.6 μm, joint efficiency stabilized at 0.96, and production yield reached 100%.

⇄0So sánhSo sánh thông số