Hydraulic components2025

Linking valve-block bore Rmr curves to port-plate wear

CX-3/160 profilometry to ISO 4287 revealed that early port-plate wear traced to insufficient bearing length in the 15° chamfer zone.

Company
Hydraulic valve block maker, Jiangsu
Address
Changzhou, Jiangsu
Linking valve-block bore Rmr curves to port-plate wear
62%Rmr(30%) restored
70%Scar depth reduction

A crescent-shaped wear scar appeared on the port plate after 500-hour bench runs, with the block supplier and pump maker blaming each other.

Solution: Ra, Rz and Rmr(30%) curves were taken at several bore depths with the CX-3/160, including the 15° chamfer transition, on new and run-in parts.

Result: Rmr(30%) in the chamfer fell from 62% to 41% — the pressure concentration was the root cause. Two-stage honing plus chamfer polishing cut the 500-hour scar depth by 70%.