Composite materials2025

Metallographic porosity sampling of CFRP laminates

MMAS-15 measured CFRP porosity per ASTM E2109 area method; a correlation with C-scan raised sampling efficiency 5x.

Company
A CFRP products manufacturer, E. China
Address
Jiangsu
Category
Microscopes
Metallographic porosity sampling of CFRP laminates
5×Inspection efficiency

CFRP drone-arm laminates were screened by ultrasonic C-scan, which is only qualitative, while the customer demanded quantitative proof of ≤1% porosity.

Solution: the MMAS-15 metallographic system applied the ASTM E2109 area method, counting pore area fraction over 20 consecutive fields at 50X (40 mm2 per specimen); C-scan grayscale over the same area was correlated to porosity.

Result: measured porosity was 0.6-0.9%, meeting the requirement. The correlation curve enables fast C-scan grading, cutting per-part inspection from 40 to 8 minutes, a 5x efficiency gain.