Additive manufacturing2024

HXZDQ-100Z Precision Cutting of AM Titanium Porosity Samples

HXZDQ-100Z low-speed precision cutting prevents burn on SLM TC4 coupons; with cold mounting and 0.05 um final polish, porosity reads a stable 0.08% by image analysis, tripling lot release efficiency.

Company
An AM service centre, E. China
Address
Shanghai
HXZDQ-100Z Precision Cutting of AM Titanium Porosity Samples
<5 μmCut burn layer
0.08%Measured porosity

SLM-built TC4 parts require porosity below 0.2%. Abrasive cut-off sampling caused a 50 um heat-tinted layer that rounded pore edges, so image analysis read 30% low and release depended on destructive tensile sampling.

Solution: an HXZDQ-100Z precision metallographic cutter with a low-speed 300 rpm diamond blade and full immersion cooling keeps the burn layer under 5 um. Vacuum-impregnated epoxy cold mounting avoids pore-fill artefacts, and polishing finishes with 0.05 um diamond suspension.

Results: on unetched polished sections, 20-field image analysis reads a stable 0.08% porosity, within 0.01 percentage points of X-ray CT. Lot release switched from tensile sampling to metallography, cutting release time from 5 days to 1.5 days.

⇄0CompareProduct comparison