Aerospace2024

In-situ hardness gradient of SX blades at 1100℃

IMAS-HT1500CM mapped in-situ hardness on 5 sections of a DD6 SX blade at 1100℃ for life-model correction.

Firma
An aero-engine materials institute, E. China
Adresse
Jiangsu
In-situ hardness gradient of SX blades at 1100℃
1100 ℃Max in-situ temperature
≤ 8%Model deviation

The institute previously extrapolated hot hardness from room-temperature data, causing over 25% deviation between blade life models and rig tests.

Solution: IMAS-HT1500CM with a 10-3 Pa vacuum chamber applied 1 kgf Vickers indents on 5 sections (root to airfoil) at 900/1000/1100℃, with 20 min soaking and in-situ 10X optical reading per GB/T 4340.1.

Result: airfoil hardness fell from 468 HV at room temperature to 285 HV at 1100℃ (-39%), with the γ′ dissolution knee near 1050℃. The life-model deviation converged to within 8% after adopting the measured curve.