Die and mold making2023

Martensite rating of quenched H13 die steel

MMAS-18 rated quenched H13 per JB/T 8420; a 25℃ overheating causing grade-4 structure was corrected, raising die life 40%.

Firma
A precision mold maker, E. China
Adresse
Shanghai
Kategorie
Microscopes
Martensite rating of quenched H13 die steel
3 万 → 11 万次Die life

A lot of H13 die-casting dies cracked thermally after only 30k shots, far below the 80k design life; microstructural evidence was needed to locate the heat-treatment fault.

Solution: the MMAS-18 system rated quenched martensite of the failed core and witness samples per JB/T 8420, grading acicular martensite at 500X and measuring retained austenite.

Result: the failed die showed grade-4 coarse martensite, corresponding to a quench temperature 25℃ over specification, with 12% retained austenite. Restoring the 1030℃ standard quench returned the structure to grade 2, and die life rose to 110k shots, a 40%+ gain.

⇄0VergleichTechnischer Vergleich