Xe năng lượng mới2025

Đo gradient độ cứng trục tôi cảm ứng

HVS-5Z đo lớp tôi cảm ứng theo GB/T 5617, HV5, sâu 2,1 mm.

Công ty
Nhà máy linh kiện điện động, Đông Trung Quốc
Địa chỉ
Ninh Ba, Chiết Giang
Đo gradient độ cứng trục tôi cảm ứng
2.1 mmĐộ sâu lớp
3 天 → 2 hThời gian kiểm tra

The EV reducer input shaft is induction hardened to a case depth of 1.8-2.5 mm with a surface of 58-62 HRC. Rockwell spot checks only saw the surface, and case depth went out for destructive metallography on a 3-day cycle, badly delaying process adjustments.

Solution: an HVS-5Z digital low-load Vickers hardness tester, HV5 (49.03 N) load with 15 s dwell, indenting radially every 0.2 mm across the shaft section to draw the hardness gradient; case depth is judged at the 550 HV limit per GB/T 5617.

Result: case depth measured 2.1 mm with a surface of 735 HV (about 61.5 HRC) and a smooth transition zone; agreement with destructive metallography was within 0.08 mm, so depth checks moved in-house.

Benefit: case-depth results come out the same day, and hardening-line response time fell from 3 days to 2 hours.

⇄0So sánhSo sánh thông số