Стальные материалы2024

Автоматическая оценка включений в стали 60Si2Mn

MMAS-100: автооценка включений по GB/T 10561, ресурс вырос на 40%.

Компания
Производитель рессорной стали, Сев. Китай
Адрес
Хэбэй
Категория
Микроскопы
Автоматическая оценка включений в стали 60Si2Mn
22 万 → 31 万次Стендовый ресурс

A lot of 60Si2Mn leaf springs failed early in bench fatigue tests, with crack origins at stringer inclusions; manual rating was slow and missed fields.

Solution: the MMAS-100 research metallographic system with a motorized stage scans the full 160 mm2 section per GB/T 10561 method A, classifying B-type (alumina) stringers by length at 100X.

Result: the failed heats rated 2.5 fine / 1.5 heavy for B-type inclusions, traced to low slag basicity in refining. After slag adjustment, ratings stabilized at 1.0 fine and bench life recovered from 220k to 310k cycles.

⇄0СравнениеСравнение характеристик