Steel materials2024

Automated inclusion rating of 60Si2Mn spring steel

MMAS-100 automatically rates B-type inclusions per GB/T 10561; tracing the slag system issue raised fatigue life by 40%.

Company
A spring steel producer, N. China
Address
Hebei
Category
Microscopes
Automated inclusion rating of 60Si2Mn spring steel
22 万 → 31 万次Bench life

A lot of 60Si2Mn leaf springs failed early in bench fatigue tests, with crack origins at stringer inclusions; manual rating was slow and missed fields.

Solution: the MMAS-100 research metallographic system with a motorized stage scans the full 160 mm2 section per GB/T 10561 method A, classifying B-type (alumina) stringers by length at 100X.

Result: the failed heats rated 2.5 fine / 1.5 heavy for B-type inclusions, traced to low slag basicity in refining. After slag adjustment, ratings stabilized at 1.0 fine and bench life recovered from 220k to 310k cycles.

⇄0CompareProduct comparison