Hardness Gradient Measurement on Nitrided Cases: White Layer, Threshold Hardness and Point Spacing

Nitrided case depth uses core hardness +50 HV or 550 HV as threshold; the brittle white layer is rated separately; gradient steps start at 0.05 mm.

华旋光电技术部
Hardness Gradient Measurement on Nitrided Cases: White Layer, Threshold Hardness and Point Spacing

Structure of the nitrided case

A gas-nitrided case has two sub-layers: the white layer (compound layer of ε-Fe₂₋₃N and γ′-Fe₄N, 5-30 μm thick, above 1000 HV but brittle) and the diffusion layer (nitrogen in ferritic solid solution plus fine alloy nitrides, 600-900 HV, falling gradually toward the core). Case depth per GB/T 11354 is the perpendicular distance from the surface to the point reading 50 HV above the core hardness; a 550 HV threshold may alternatively be agreed, consistent with carburizing practice.

Gradient measurement parameters

Use micro-Vickers HV0.1-HV0.3, and HV0.025-HV0.05 for the thin white layer. Step points along the cross-section at 0.05 mm within the first 0.2 mm, relaxing to 0.1 mm deeper; keep indent spacing and surface distance at least 2.5 diagonals. Determine core hardness before nitriding as the threshold baseline. Take at least 8-10 points per column and average three columns; column spread beyond 0.05 mm signals uneven nitriding.

Evaluating the white layer

Thicker is not better: beyond 30 μm, or with visible porosity, the white layer spalls in service. The evaluation covers thickness (metallographic), brittleness (crack rating 1-4 from the corner cracks of an HV10 indent, 1 best) and phase constitution (ε/γ′ ratio by XRD). Precision gears and dies typically require a white layer of 15 μm or less, or specify grinding it off.

Common data problems

First, an anomalous dip at the surface usually means the white layer was ground away or indents landed in a porous band. Second, a long plateau near the threshold indicates a flat nitrogen gradient — a process issue, not a measurement issue. Third, core hardness taken at the wrong depth: measure it unaffected by nitrogen, deeper than three times the case depth. A complete report states case depth, threshold convention, load and core hardness — all four.