Aerospace2025

In-situ 1600 °C hardness and interface cracking of TBC

The HMAS-UHT1700CM indented the ceramic top coat in-situ at 1600 °C through the 10× objective, reading crack lengths directly instead of cooling-guess work.

회사명
Aero-materials research institute, East China
주소
Shanghai
In-situ 1600 °C hardness and interface cracking of TBC
1600 ℃Max in-situ temperature
R² 0.92Life correlation

Previous practice measured hardness at room temperature and extrapolated, and interface-toughness data deviated badly from rig results.

Solution: HMAS-UHT1700CM in a glovebox (H₂O/O₂ ≤1 ppm), 1 kgf constant-force indents after 30-minute soaks at 800/1000/1200/1400/1600 °C, with in-situ 10× imaging of indentation and interface cracks, three indents per point.

Result: top-coat hardness fell from 620 HV at 800 °C to 410 HV at 1600 °C with a softening knee matching TGO growth; interface KIC 4.3 MPa·m1/2 correlated with thermal-cycling life at R² = 0.92.