Hardmetals2024

Sintering window of WC-Co defined by hardness at 1000 °C

Hardness at 1000 °C on HMAS-HT900CM replaces eight high-temperature bend runs and cuts sintering-window validation from three weeks to four days, resolving 20 °C furnace differences.

회사명
Hardmetal producer, Zhuzhou
주소
Zhuzhou, Hunan
Sintering window of WC-Co defined by hardness at 1000 °C
3 周 → 4 天Validation time
20 ℃Temperature resolution
R² 0.88Vs. bend test

The plant runs WC-10Co and WC-6Co grades with a ±15 °C sintering window; overheating brings η phase and abnormal grain growth. The traditional route ran a high-temperature three-point bend set (five parts) per temperature, eight points in three weeks, with large scatter.

Solution: one specimen per sintering temperature on HMAS-HT900CM, argon atmosphere, 1000 °C with a 10 min soak, five HV5 indents and mean plus range; one bend set kept for correlation.

Result: full window mapped in four days; sensitivity about 12 HV per 10 °C, enough to resolve 20 °C; correlation with bend strength 0.88, so routine checks now use hot hardness and bends are reserved for new grades, saving roughly CNY 300k per year.