Semiconductor2024

In-line rapid hardness sampling of lead-frame copper strip

W-B75 clamp-type Webster tester samples C194 copper strip hardness in line in 3 seconds without damaging the strip; 9.5-10.5 HW corresponds to about 125 HV, replacing lab sampling.

会社名
A lead-frame material plant, E. China
所在地
Suzhou, Jiangsu
カテゴリ
Hardness Testers
In-line rapid hardness sampling of lead-frame copper strip
3 sTime per reading
每周 → 每卷Check frequency

The aged hardness of C194 copper-alloy strip governs stamping burrs on lead frames. Lab Vickers checks ran weekly with results three days late, so off-hardness lots had often already stamped hundreds of thousands of pieces.

Solution: a W-B75 clamp-type Webster hardness tester (copper-alloy model) clamps 0.2-0.4 mm strip directly on the slitting line; three seconds per reading with a tiny indentation that does not affect downstream processing. An HW-to-HV conversion table goes out with the process documents, cross-checked against lab micro-Vickers data quarterly.

Result: in-line readings of 9.5-10.5 HW (about 125 HV) agreed with lab HV0.2 within 5%; one lot reading 0.8 HW low was intercepted immediately.

Benefit: hardness monitoring moved from weekly to every coil, and burr-related batch scrap has not recurred.