Semiconductor packaging2025

Void-rate sectioning of BGA joints and reflow optimization

BID-500 sectioned BGA joints per IPC-A-610; lowering peak reflow by 8℃ cut void rate from 18% to 9%.

Company
A chip packaging and test house, S. China
Address
Guangdong
Category
Microscopes
Void-rate sectioning of BGA joints and reflow optimization
18% → 9%Void rate

X-ray showed elevated voiding in a BGA lot (some joints >25%); the customer demanded sectioning data plus corrective actions.

Solution: the BID-500 system applied IPC-A-610 step-sectioning: grinding along the diagonal to joint mid-sections, void area fraction measured at 200X on 12 corner joints per device, with a reflow-profile DOE in parallel.

Result: sectioning gave an 18% mean void rate. Lowering peak temperature from 250℃ to 242℃ and extending soak by 15 s cut voiding to 9%; all joints passed the 25% acceptance line.