How to avoid cutting burn?

Choose the right blade, ensure copious coolant aimed at the cut, and reduce feed rate. Burn appears as a white layer that polishing cannot remove.

Hot or cold mounting?

Hot mounting is fast with good edge retention; cold mounting suits heat-sensitive or coated samples. Use vacuum impregnation for porous or coated interfaces.

What grinding/polishing sequence?

180 → 400 → 800 → 1200 grit, each perpendicular to the previous, then 3 µm and 1 µm diamond followed by 0.05 µm silica. Reduce pressure on soft metals.

How to choose an etchant?

Nital for carbon and low-alloy steels, aqua regia for stainless, Keller for aluminium, ferric chloride for copper alloys. Start dilute and short, stop at clear grain boundaries.

How to troubleshoot preparation defects?

Scratches mean incomplete previous step or dirty cloth; comet tails need lower pressure; relief needs shorter high-pH polishing; rounded edges need better mounting.