Bài kỹ thuật641 lượt xem

Đo gradien độ cứng vi mô của lớp phủ: tải, bước đo và hiệu chỉnh nền

Lớp phủ ~20 μm cần tải ≤HV0.05, khoảng cách vết ấn ≥2,5 đường chéo và hiệu chỉnh hiệu ứng nền gần biên.

华旋光电技术部
Đo gradien độ cứng vi mô của lớp phủ: tải, bước đo và hiệu chỉnh nền

Load selection

The first constraint in coating gradient measurement is that the indent must fit inside the layer: coating thickness should be at least 1.5 times the indentation diagonal, following the thickness requirement of GB/T 4340.1, otherwise the reading is a composite of coating and substrate. For a 20 μm PVD TiN coating the diagonal must stay within about 13 μm, corresponding to loads of HV0.025 to HV0.05; a 50 μm thermal-sprayed layer allows HV0.1 to HV0.3. Smaller is not always better: below a 20 μm diagonal the measurement error grows steeply, and the diagonal reading resolution of the tester should be better than 0.2 μm.

Indent spacing rules

Indent along the cross-section normal to the surface. The spacing between adjacent indent centers should be at least 2.5 mean diagonals, and the indent edge should be at least 2.5 diagonals away from the free surface and the interface. A step of one eighth to one tenth of the layer thickness is recommended, giving at least ten points across a 100 μm diffusion layer. Two or three parallel indents per depth, averaged, suppress scatter from local microstructure. Mounting the specimen at a shallow taper angle of 1 to 2 degrees effectively magnifies depth resolution; the true depth then equals the measured value multiplied by sin θ.

Substrate-effect correction

When the plastic zone reaches into the substrate near the interface, readings shift toward the substrate value. Composite hardness models such as the Bückle weighting H_c=H_f·(2a/t·sin(11°)) + H_s·(1-2a/t·sin(11°)) can separate film hardness H_f from the composite value H_c, with a the half-diagonal and t the film thickness. A simpler engineering practice is to plot hardness versus depth, take the plateau as the true film hardness, and use the transition zone only qualitatively.

Reporting

A gradient report should state load, dwell time (10 to 15 s), the coordinates of each indent, measured diagonals and converted hardness, with the coating surface as depth zero. For coatings serving at high temperature, such as bond coats on turbine blades, key points should be re-measured at service temperature on a hot microhardness tester: a diffusion aluminide reading 900 HV at room temperature may fall below 300 HV at 900 °C, and the gradient shape itself rearranges.

⇄0So sánhSo sánh thông số