HXQ-50 ép mẫu mặt cắt đầu cos

HXQ-50 ép mẫu 180°C/25 MPa mặt cắt đầu cos; nén 82%, rỗng 3%, chu kỳ 12 phút.

Công ty
Nhà máy đầu nối ô tô, Nam Trung Quốc
Địa chỉ
Thâm Quyến, Quảng Đông
HXQ-50 ép mẫu mặt cắt đầu cos
82%Tỷ lệ nén dây
12 minChu kỳ phân tích

Crimp quality on automotive terminals was checked only by pull tests - internal voids and wire compression were invisible, so die wear was found only at failure, and over-resistance crimps once escaped in volume.

Solution: an HXQ-50 automatic hot mounter embeds Φ0.5 mm terminals at 180°C and 25 MPa for 5 minutes without collapsing the crimp. Sections polished to 1 um are read at 100X for wire compression ratio, porosity and wing engagement; three sections per shift.

Results: compression holds at 82% with 3% porosity, and trend data warns of crimp die wear two weeks early. Over-resistance escapes went to zero, section analysis runs at 12 minutes per piece, and about 900000 yuan of claims are avoided a year.