技術資料461 views

Differential Interference Contrast (DIC): From Optical Path Difference to Relief Images

A Nomarski prism shears the beam in two; nanometre surface steps become optical path differences and appear as relief, revealing details invisible in brightfield.

华旋光电技术部
Differential Interference Contrast (DIC): From Optical Path Difference to Relief Images

Optical principle

DIC in a reflected-light metallurgical microscope combines a polarizer, a Nomarski-modified Wollaston prism and an analyzer. Linearly polarized light from the polarizer is sheared by the prism into two beams with orthogonal vibration directions, laterally offset by a sub-micron distance, striking two neighboring surface points. After reflection the beams recombine in the prism and interfere through the analyzer. A surface step Δh introduces an optical path difference of 2Δh, i.e. a phase difference δ=4πΔh/λ, which converts into brightness — this is how DIC turns height information into grey levels.

Image character and adjustment

A DIC image shows directional relief: height changes along the shear direction appear as bright-dark contrast, while edges perpendicular to the shear almost vanish, so rotate the specimen for the best orientation. Rotating the prism shifts the bias retardation; tuning the background from grey to magenta (the sensitive tint) maximizes sensitivity near zero order, resolving surface undulations of 1 to 2 nm, far beyond brightfield.

Typical applications

  • Unetched microstructure: ferrite and pearlite develop micro-relief from hardness differences during polishing, separable in DIC without etching;
  • Inclusion-matrix interfaces: oxide and sulfide boundaries show strong contrast, making fine inclusions easier to spot than in brightfield;
  • Polishing quality control: fine scratches and relief invisible in brightfield stand out in DIC, making it an acceptance tool for high-grade preparation;
  • Martensitic surface relief: transformation-induced upheaval can be observed directly for phase-transformation studies.

Practical notes

DIC needs dedicated objectives with DIC slots and matched prisms; stress birefringence in ordinary brightfield objectives degrades contrast. Set the polarizer and analyzer to accurate extinction or sensitivity drops sharply. The specimen must be polished to high quality, since heavy scratches generate chaotic fringes that mask the structure. Remember that DIC contrast is gradient contrast, not true height; quantitative height measurement still belongs to interferometers or profilometers.

⇄0比較仕様比較