よくある質問

よくある質問

選定ガイド · 試験方法

OES vs handheld XRF?

OES measures C, S, P, N with high precision but needs argon and prepared samples; XRF is portable and non-destructive but blind to light elements. Use both for different jobs.

How should samples be prepared?

Representative sampling, then grind flat with 60–120 grit alumina, avoiding scratches and overheating. Soft metals such as Al and Mg should be milled, not ground.

How often to standardise?

Type standardisation every shift or 2 hours; full standardisation weekly or after service. Always re-standardise after changing argon or cleaning the lens.

What happens with impure argon?

Oxygen, nitrogen and moisture blacken the burn spot and depress light-element results. Use 5N purity, dew point ≤-60°C and stainless or copper lines.

What detection limits are achievable?

Typically ppm level for common elements, sub-ppm with high-resolution systems. Ask for 3σ measured values on your matrix.