Cemented carbide R&D2024

Rapid 1000℃ hardness screening of WC-Co grades

HMAS-HT1300CM screened 12 WC-Co compositions at 1000℃ in one day, replacing two weeks of work; 6% Co was identified as optimum.

Company
A cemented carbide institute, SW China
Address
Sichuan
Rapid 1000℃ hardness screening of WC-Co grades
12 牌号 / 8 hScreening throughput

When developing tool substrates for high-speed cutting, the institute needed to compare hardness retention at cutting temperature across 12 Co contents (4-10%), but conventional furnaces allowed only 2-3 temperature points per day.

Solution: HMAS-HT1300CM with a 12-position carousel applied five 1 kgf indents per sample at 1000℃ in argon, 10 s dwell, with in-situ diagonal reading through a 20X long-working-distance objective, cross-checked against GB/T 4340.1 and ISO 6507.

Result: the 6% Co grade showed the best retention (1780 HV at RT to 890 HV at 1000℃, 50%). The full screening finished within 8 hours, shortening the development cycle by about 40%.

⇄0CompareProduct comparison